- Home |
- Technical Data |
- Heat Treatments |
- AISI - 1050 - SAE
AISI - 1050 - SAE
| Formed Springs Requiring Heat Treatment AISI - 1050 - SAE |
|||
| Normal Temp | 1550° - 1650° F. | ||
| Anneal Temp | 1400° - 1500° F. | ||
| Hard Temp | 1500° - 1550° F. | ||
| Oil Quench | Rc 58 | ||
| Rockwell Drawing Temp. * AISI - 1050 - SAE |
|||||||
| 400° F | 600° F | 700° F | 800° F | 900° F | 1000° F | 1100° F | 1200° F |
| Rc 52 | Rc 45 | Rc 39 | Rc 35 | Rc 31 | Rc 27 | Rc 22 | N/A |
| Tensile PSI Drawing Temp. * AISI - 1050 - SAE |
|||||||
| 400° F | 600° F | 700° F | 800° F | 900° F | 1000° F | 1100° F | 1200° F |
| 250,000 | 210,000 | 180,000 | 160,000 | 139,000 | 124,000 | 112,000 | N/A |
Special Note - These temperature ranges and their resultant values are given as information only and not to be followed without experimentation. However, as these steels are held to close uniformity tolerances little difficulty should be experienced.